タイトル | Solid State Electrolytes Prepared from PEO (360) Silanated Silica |
本文(外部サイト) | http://hdl.handle.net/2060/20020070846 |
著者(英) | Liu, B.; Maitra, P.; Salomon, M.; Wunder, S. L.; Ding, J.; Chua, D.; Lin, H.-P. |
著者所属(英) | MaxPower, Inc.|Temple Univ. |
発行日 | 2002-01-01 |
言語 | eng |
内容記述 | All solid state composite electrolytes were prepared using fumed silica (SiO2) silanated with an oligomeric polyethylene oxide (PEO) silane containing 6-9 ethylene oxide repeat units, a PEO matrix and LiClO4 (8/1 O/Li). The PEO-silane covalently attached to the silica was amorphous, with a T(sub g) that increased from -90 C to -53 C after attachment. The conductivity of films prepared using the PEO-silanated silica increased to approx. 6 x 10(exp -5) S/cm at RT compared with approx. 1 x 10(-5) S/cm for films prepared with unsilanated SiO2. |
NASA分類 | Spacecraft Propulsion and Power |
権利 | No Copyright |
URI | https://repository.exst.jaxa.jp/dspace/handle/a-is/224503 |
|